DIN |
AISI | JIS |
GB |
1.2344 |
H13 | SKD61 |
4Cr5MoSiV1 |
Chemical Composition(DIN 17350)
C |
Si |
Mn |
P≤ |
S≤ |
Cr |
Mo |
V |
0.37 |
0.90 |
0.30 |
0.030 |
0.030 |
4.80 |
1.20 |
0.90 |
0.42 |
1.20 |
0.50 |
5.50 |
1.50 |
1.10 |
Steel Properties
Secondary hardening steel.Good tempering resistance. It maintains high hardness and strength at elevated temperatures. Resistance to thermal fatigue, erosion and water.Very high toughness. Good ductility and hardenability-air cooling. Tools can be water cooled.Following NADCA standard.
Applications
Wear resisting tools,pressure die casting tools,pressing tools for light and heavy metal.Charpy V-Notch tested,impact toughness in ft-lbs (J) min.8 (11) for ESR;Min.10 (13.8) for premium.
Heat Treatment
Soft Annealing(℃) |
Cooling |
Hardness(HB) |
Hardening( ℃ ) |
In |
Hardness(HRC) |
760-810 |
Furnace |
Max.229 |
1020-1060 |
In air,oil,thermal
bath 450 -550 ℃ |
52-56 HRC |
Tempering (℃) |
100 |
200 |
300 |
400 |
450 |
500 |
550 |
600 |
650 |
700 |
HRC |
53 |
52 |
51 |
52 |
53 |
54 |
53 |
50 |
43 |
31 |
N/mm2 |
1845 |
1790 |
1730 |
1790 |
1845 |
1910 |
1845 |
1680 |
1360 |
995 |
|